Automotive Parts and Materials Corrosion Test Methods
This standard revises JASO M 609 (Corrosion Test Methods for Automotive Materials) and JASO M 610 (Test Methods for Automotive Parts Appearance Corrosion) by reclassifying the test types for appearance corrosion and pitting corrosion in order to improve correlation with the actual corrosion conditions of automobiles in the market.
The standard specifies a method for determining the corrosion resistance (exterior corrosion and pitting corrosion) of steel materials used for automobiles and automotive parts and materials made of steel materials with surface treatment on the base material by a combined cycle test.
The test has been split into two new methods, covering two applications
- Apperance Corrosion – Cycle Method A or B
 
- Perforated Corrosion – Cycle Method C
 
The test method consists of repeatedly exposing the specimens to salt water, dry and wet atmospheres under specified conditions, and evaluating the appearance corrosion of parts and materials, pitting corrosion in mating parts, etc. The test is performed by repeatedly exposing the specimens to salt water, dry and wet atmospheres in sequence.
Test Method B has been split into two test applications
- Salt Spray Method (salt atomisation)
 
- Salt Shower Method (overhead oscillating salt spray)
 
Here we discuss the 2nd application for Salt Shower Method
Method B Salt Spray Method Test Conditions
| Method B | 
Function | 
Duration | 
Transistion included in duration | 
| 1 | 
Salt Spray 50℃ +/-1℃ | 
15 mins | 
1 hour | 
| 2 | 
Drying 60℃ +/-1℃ & 50 %RH±5 %RH | 
8 hours | 
30 min | 
| 3 | 
Wetting 50℃ +/-1℃ & 95 %RH or above | 
4 hours | 
1 hour | 
| 4 | 
Drying 60℃ +/-1℃ & 50 %RH±5 %RH | 
7h 45mins | 
30 min | 
| 5 | 
Wetting 50℃ +/-1℃ & 95 %RH or above | 
4 hours | 
30 min back to step 1 | 
 | 
 | 
 | 
 | 
 | 
 | 
 | 
 | 
 | 
 | 
 | 
 | 
 | 
Fallout After a 5-minute saltwater shower collection at a rate of 15 ml to 75 ml/5 min/80 cm² | 
 | 
 | 
This test is also referred to as a Cyclic Corrosion Test, often abbreviated to CCT.
<!– To select an Ascott chamber suitable for this test click here –>
	 
	
	
	
		Automotive Parts and Materials Corrosion Test Methods
This standard revises JASO M 609 (Corrosion Test Methods for Automotive Materials) and JASO M 610 (Test Methods for Automotive Parts Appearance Corrosion) by reclassifying the test types for appearance corrosion and pitting corrosion in order to improve correlation with the actual corrosion conditions of automobiles in the market.
The standard specifies a method for determining the corrosion resistance (exterior corrosion and pitting corrosion) of steel materials used for automobiles and automotive parts and materials made of steel materials with surface treatment on the base material by a combined cycle test.
The test has been split into two new methods, covering two applications
- Apperance Corrosion – Cycle Method A or B
 
- Perforated Corrosion – Cycle Method C
 
The test method consists of repeatedly exposing the specimens to salt water, dry and wet atmospheres under specified conditions, and evaluating the appearance corrosion of parts and materials, pitting corrosion in mating parts, etc. The test is performed by repeatedly exposing the specimens to salt water, dry and wet atmospheres in sequence.
Test Method B has been split into two test applications
- Salt Spray Method (salt atomisation)
 
- Salt Shower Method (overhead oscillating salt spray)
 
Here we discuss the 1st application for Salt Spray Method
Method B Salt Spray Method Test Conditions
| Method B | 
Function | 
Duration | 
Transistion included in duration | 
| 1 | 
Salt Spray 50℃ +/-1℃ | 
1 hour | 
1 hour | 
| 2 | 
Drying 60℃ +/-1℃ & 50 %RH±5 %RH | 
8 hours | 
30 min | 
| 3 | 
Wetting 50℃ +/-1℃ & 95 %RH or above | 
4 hours | 
1 hour | 
| 4 | 
Drying 60℃ +/-1℃ & 50 %RH±5 %RH | 
7 hours | 
30 min | 
| 5 | 
Wetting 50℃ +/-1℃ & 95 %RH or above | 
4 hours | 
30 min back to step 1 | 
 | 
 | 
 | 
 | 
 | 
 | 
 | 
 | 
 | 
 | 
 | 
 | 
 | 
Fallout requirement is 1-2ml per 80cm² per hour | 
 | 
 | 
Chamber volumes of less than 400 Litres are not permitted by this test standard.
This test is also referred to as a Cyclic Corrosion Test, often abbreviated to CCT.
<!– To select an Ascott chamber suitable for this test click here –>
	 
	
	
	
		Automotive Parts and Materials Corrosion Test Methods
This standard revises JASO M 609 (Corrosion Test Methods for Automotive Materials) and JASO M 610 (Test Methods for Automotive Parts Appearance Corrosion) by reclassifying the test types for appearance corrosion and pitting corrosion in order to improve correlation with the actual corrosion conditions of automobiles in the market.
The standard specifies a method for determining the corrosion resistance (exterior corrosion and pitting corrosion) of steel materials used for automobiles and automotive parts and materials made of steel materials with surface treatment on the base material by a combined cycle test.
The test has been split into two new methods, covering two applications
- Apperance Corrosion – Cycle Method A or B
 
- Perforated Corrosion – Cycle Method C
 
The test method consists of repeatedly exposing the specimens to salt water, dry and wet atmospheres under specified conditions, and evaluating the appearance corrosion of parts and materials, pitting corrosion in mating parts, etc. The test is performed by repeatedly exposing the specimens to salt water, dry and wet atmospheres in sequence.
Method A Test Conditions
| Method A | 
Function | 
Duration | 
Transistion included in duration | 
| 1 | 
Salt Spray 50℃ +/-2℃ | 
10 min | 
30 min | 
| 2 | 
Drying 60℃ +/-2℃ & Less than 30%RH | 
2h 35min | 
30 min | 
| 3 | 
Wetting 60℃ +/-2℃ &95 %RH±5 %RH | 
1h 15 min | 
30 min | 
| 4 | 
Drying 60℃ +/-2℃ & Less than 30%RH | 
2h 40min | 
30 min | 
| 5 | 
Wetting 60℃ +/-2℃ & 95 %RH±5 %RH | 
1h 20 min | 
10 min back to step 1 | 
 | 
 | 
 | 
 | 
 | 
Repeat steps 4&5  for 5 times before starting cycle again | 
 | 
 | 
 | 
 | 
 | 
 | 
 | 
Fallout requirement is 1-2ml per 80cm² per hour | 
 | 
 | 
Chamber volumes of less than 400 Litres are not permitted by this test standard.
This test is also referred to as a Cyclic Corrosion Test, often abbreviated to CCT.
<!– To select an Ascott chamber suitable for this test click here –>
	 
	
	
	
		Mazda MES MN 601G  Test Method for Paint Film
Section 27 for this test standard discusses the 5 class requirements for corrosion testing
Class 1 – Salt Spray Test
Class 2 – Perforation Corrosion Resistance Test
Class 3 – Scratch Corrosion Resistance Test
Class 4 – Edge Corrosion Resistance Test
Class 5 – Filiform Corrosion Resistance Test
Class 2 OR Class 3 can be tested to MAZDA MCT-2M which requires a fully enclosed chamber to perform the following test steps:
- 6 hour Salt Spray @ 35°C in accordance with JIS Z 2371
 
- 3 hours Drying @ 50°C /  20-40%RH
 
- 14 Hour wetting @ 50°C / 95% RH
 
- 1 hour standard ambient temperature
 
The test profile runs for 24 hours
For Class 2 testing this should be ran for 120 cycles
For Class 3 testing this should be ran for 60 cycles
This test can be ran in an Ascott Cyclic Chamber fitted with some accessories
	 
	
	
	
		Nissan Engineering Standard – Composite Corrosion Test
NES M-0007 is used to measure the degree of rusting, blistering and adhesion when the specimen is exposed to corrosive conditions such as salt spray, drying and wetting (condensate humidity)
Method B of the standard requires a Cyclic corrosion chamber which can automatically cycle between periods of salt spray, drying and wetting.
Any one of the following cycles below can be chosen to run this test in agreement with the parties concerned
- CCT-1 -Salt Spray (35°C, 4h) → drying (60°C, 2h)→ wetting (50°C, 95% RH, 2h)
 
- CCT-2- Salt Spray (35°C, 2h) → drying (60°C, 2h)→ wetting (50°C, 95% RH, 4h)
 
- CCT-4 -Salt Spray (35°C, 10min) → drying (60°C, 155min)→ wetting (60°C, 95% RH, 75min), with a sub-programme of drying (60°C, 160min)→wetting (60°C, 95%RH, 80min) repeated 5 times
 
See above hyperlinks for further information on each of these test methods
	 
	
	
	
		Nissan Engineering Standard – Salt Spray Testing
Nissan MES-M0007  is used to measure the degree of rusting, blistering and adhesion when the specimen is exposed to corrosive conditions such as salt spray, drying and wetting (condensate humidity)
Method A of the standard requires salt spray testing in accordance with NES M-0140 whereby test specimens are placed in an enclosed chamber and exposed to a continuous indirect spray of neutral (pH 6.5 to 7.2) salt water solution, which falls-out on to the specimens at a rate of 1.0 to 2.0ml/80cm²/hour, in a chamber temperature of +35C. This climate is maintained under constant steady state conditions. The test duration is variable.
This test is also referred to as an NSS test.
	 
	
	
	
		Nissan NES M0158 – Methods of Compound Corrosion Test
This Nissan engineering standard specifies the method to measure compound corrosion that uses the combined processes of salt spraying or salt solution immersion followed by drying and moistening. The process will simulate and accelerate corrosion of metal materials used on automobiles. Therefore this test will measure corrosion of metals of functional decorative parts together with the coating effect of inorganic or organic plating of vehicle models.
It is an accelerated laboratory corrosion test method that can be used to determine the corrosion resistance of automotive assemblies and components. It is cyclic in nature, i.e.; test specimens are exposed to changing climates over time.
As a rule, the testing equipment shall have the ability to generate and automatically repeat 3 different processes, i.e. salt solution spraying or immersion, drying and moistening.
- CCT-I Corrosion resistance in general (surface rust and penetrated rust): Vehicle body panel, road wheel, under-floor piping, drive shaft, propeller shaft, fastening parts (bolts and nuts) etc.
 
- CCT-IV External panel scab rust: External panel, external topcoat
 
- CCT-V Internally accelerated penetration of rust: Internal panel, box structure parts
 
See the hyperlinks above for information on each individual test standard
	 
	
	
	
		Nissan NES M0158 – CCT 5 (CCT-V)
This Nissan engineering standard specifies the method to measure compound corrosion that uses the combined processes of salt spraying or salt solution immersion followed by drying and moistening. The process will simulate and accelerate corrosion of metal materials used on automobiles. Therefore this test will measure corrosion of metals of functional decorative parts together with the coating effect of inorganic or organic plating of vehicle models.
It is an accelerated laboratory corrosion test method that can be used to determine the corrosion resistance of automotive assemblies and components. It is cyclic in nature, i.e.; test specimens are exposed to changing climates over time.
Test specimens are placed in an enclosed chamber and exposed to a changing climate that comprises of a relatively short period of salt immersion, followed by exposure to hot/humid and hot/dry atmospheres.  1 entire test cycle takes 2 hours to execute. The number of entire cycle repeats and therefore the test duration is variable.
The main test cycle begins with 5 minutes salt water immersion at 60°C  followed by 55 minutes of drying at 80°C , Humidity less than 30%rh . The final step is wetting at 60°C / 95%RH for 1 hour.
The total cycle is 2 hours and repeatable
The atmosphere in the chamber must be “instant setting” with a transition time of less than 10 seconds, and 1 cycle should take 2 hours. However, the process of Drying → Moistening should take less than 30 minutes.
	 
	
	
	
		Mazda MES MN 601G  Test Method for Paint Film
Section 27 for this test standard discusses the 5 class requirements for corrosion testing
Class 1 – Salt Spray Test
Class 2 – Perforation Corrosion Resistance Test
Class 3 – Scratch Corrosion Resistance Test
Class 4 – Edge Corrosion Resistance Test
Class 5 – Filiform Corrosion Resistance Test
Class 3-4 are commonly referred to as MAZDA MCT-3M which requires a fully enclosed chamber to perform the following test steps:
- 1 hour Salt Spray @ 35°C in accordance with JIS Z 2371
 
- 6 hours Drying @ 60°C /  10-30%RH
 
- 1 Hour wetting @ 50°C / 95% RH
 
The test profile runs for 8 hours and 180 cycles
This test can be ran in an Ascott Cyclic Chamber fitted with accessories ACC42 & ACC47
	 
	
	
	
		Cosmetic Corrosion Test Method for Automotive Parts
This standard specifies a test method for examining the cosmetic corrosion of metallic automotive parts and their surface treatments. It is cyclic in nature, i.e.; test specimens are exposed to changing climates over time.
Test specimens are placed in an enclosed chamber and exposed to a changing climate that comprises of the following 3 part repeating cycle. 2.0 hours exposure to salt spray at +35C according JIS Z 2371. This is followed by 4.0 hours of air drying in a climate of 20 to 30%RH at +60C. This is followed by 2.0 hours exposure to a condensing water climate (wetting) of 95 to 100%RH at +50C. The number of cycle repeats and therefore the test duration is variable.
The maximum transition times between each part of the test cycle are also specified as follows:
From salt spraying to air drying within 30 minutes.
From air drying to wetting within 15 minutes.
From wetting to salt spraying within 30 minutes.
Please see elsewhere in this document for details of JIS Z 2371.
Chamber volumes of less than 400 Litres are not permitted by this test standard.
This test is also referred to as a Cyclic Corrosion Test, often abbreviated to CCT.