Hyundai CCT-D (MS600-66)

Hyundai/Kia  CCT-D

An accelerated corrosion test under complex environment shall be performed in accordance with CCT-D of MS600-66

Step 1: Salt Dipping (Immersion) @ 50°C  for 2 hours

Step 2: Wetting @ 50°C / 95%RH for 8 hours

Step 3: Drying @ 70°C / 30%RH for 1.5 hours

Step 4: Drying @ 70°C / 15%RH for 1.5 hours

Step 5: Wetting @ 35°C / 100%RH for 6.5 hours

Step 6: Drying @ 35°C / 15%RH for 2 hours

Step 7: Salt Spray @ 35°C / 95%RH for 30 minutes

Step 8: Freezing @ -20°C for 20 minutes

Transition times:

From step 1 to step 2 = 30 minutes

From step 2 to step 3 = 20 minutes

From step 3 to step 4 = 20 minutes

From step 4 to step 5 = 50 minutes

From Step 5 to step 6 = 50 minutes

From Step 6 to step 7 = 20 minutes

From Step 7 to step 8 = 60 minutes

From Step 8 to step 1 = 20 minutes

The entire cycle is 24 hours and repeatable